PHYSICAL PROPERTIES OF STEEL
These properties are approximate.
They are listed here only as a guide to
what may be expected from the grades given.
|
A.I.S.I.
No. |
Condition |
Tensile
Strength
Lb. per
Sq. In. |
Yield
Point
or Yield
Strength (1)
Lb. per
Sq. In.
|
Elong.
2" per
Center
|
Reduction
of Area
Percent |
Brinell |
| C-1008 |
Hot Rolled |
45000/55000 |
26000 |
45 |
65 |
90/124 |
| |
Cold Drawn |
52000/62000 |
49000 |
30 |
55 |
114/143 |
| C-1010 |
Hot Rolled |
48000/58000 |
30000 |
38 |
65 |
95/134 |
| |
Cold Drawn |
55000/65000 |
50000 |
25 |
52 |
124/162 |
| C-1015 |
Hot Rolled |
50000/70000 |
32000 |
35 |
60 |
105/143 |
| |
Cold Drawn |
62000/77000 |
65000 |
19 |
50 |
124/171 |
| C-1016 |
Hot Rolled |
52000/70000 |
32000 |
35 |
60 |
105/143 |
| |
Cold Drawn |
65000/80000 |
65000 |
19 |
50 |
133/171 |
| C-1017 |
Hot Rolled |
50000/70000 |
32000 |
35 |
60 |
105/143 |
| C-1018 |
Cold Drawn |
72000/85000 |
62000 |
20 |
54 |
168/168 |
| C-1019 |
Hot Rolled |
52000/70000 |
32000 |
35 |
60 |
105/143 |
| |
Cold Drawn |
65000/80000 |
65000 |
19 |
50 |
133/171 |
| C-1020 |
Hot Rolled |
54000/70000 |
32000 |
35 |
60 |
109/152 |
| |
Cold Drawn |
66000/81000 |
67000 |
18 |
50 |
133/181 |
| C-1022 |
Hot Rolled |
55000/70000 |
32000 |
35 |
55 |
114/153 |
| |
Cold Drawn |
67000/82000 |
69000 |
17 |
50 |
143/190 |
| C-1025 |
Hot Rolled |
60000/75000 |
35000 |
30 |
55 |
124/171 |
| |
Cold Drawn |
70000/85000 |
70000 |
17 |
50 |
143/190 |
| C-1030 |
Hot Rolled |
65000/80000 |
38000 |
30 |
55 |
133/181 |
| |
Cold Drawn |
75000/90000 |
75000 |
15 |
45 |
152/200 |
| |
Draw 1000°F |
90000 |
65000 |
20 |
60 |
162/219 |
| C-1035 |
Hot Rolled |
70000/85000 |
43000 |
25 |
50 |
143/190 |
| |
Cold Drawn |
80000/100000 |
80000 |
12 |
45 |
171/209 |
| |
Draw 1000°F |
95000 |
68000 |
18 |
55 |
181/228 |
| C-1040 |
Hot Rolled |
75000/90000 |
48000 |
25 |
45 |
152/190 |
| |
Cold Drawn |
85000/105000 |
80000 |
11 |
40 |
181/219 |
| |
Draw 1000°F |
100000 |
62000 |
22 |
50 |
200/247 |
| C-1045 |
Hot Rolled |
80000/95000 |
50000 |
25 |
40 |
162/200 |
| |
Cold Drawn |
90000/110000 |
85000 |
10 |
40 |
190/228 |
| |
Draw 1000°F |
100000 |
65000 |
20 |
45 |
209/247 |
| C-1050 |
Hot Rolled |
90000/110000 |
55000 |
20 |
35 |
171/228 |
| |
Cold Drawn |
100000/120000 |
90000 |
10 |
35 |
200/247 |
| |
Draw 1000°F |
115000 |
75000 |
17 |
40 |
219/266 |
| C-1095 |
Hot Rolled |
140000 |
75000 |
8 |
10 |
296/296 |
| |
Draw 1000°F |
175000 |
120000 |
10 |
20 |
375/375 |
| B-1010 |
Hot Rolled |
50000/70000 |
35000 |
35 |
55 |
101/140 |
| |
Cold Drawn |
65000/80000 |
60000 |
17 |
50 |
131/170 |
| C-1115 |
Hot Rolled |
55000/70000 |
40000 |
35 |
55 |
107/146 |
| |
Cold Drawn |
65000/80000 |
60000 |
20 |
50 |
140/179 |
| C-1117 |
Hot Rolled |
52000/67000 |
35000 |
35 |
55 |
109/153 |
| |
Cold Drawn |
70000/85000 |
65000 |
21 |
45 |
143/179 |
| C-1118 |
Hot Rolled |
55000/72000 |
40000 |
35 |
55 |
109/153 |
| |
Cold Drawn |
70000/90000 |
65000 |
19 |
45 |
143/179 |
| C-1120 |
Hot Rolled |
55000/70000 |
32000 |
35 |
55 |
109/153 |
| (1) Yield Strength for Cold Drawn. |